1、各類鋼材回火參數(shù)回火后洛氏硬度與回火溫度對照表鋼號回火后洛氏硬度(HRC與回火溫度C)的關(guān)系備注25-3030-3535-4040-4545-5050-5555-60> 6030350300200V 160以下為碳素35520460420350290V 170及低合金鋼40540490430370310V 20045550520450380320300180505605304603903303101806058054046040036031025018030Mn49040035030020040Mn54020040M n254042037032027024050M n2600480400

2、30035SiMr*56052046040035020042M n2V60052047043035020040Cr580510470420340200V 16045Cr620530480420340P 200V 18050Cr650570480400280230V 18040CrSi*63055052045040033022040CrMn*58051023020030CrM nSi*620530500430340P 18040CrV64056050045032020045CrV64056050045032020050CrV650560500450380r 28018030CrMo5604404

3、0020035CrMo60055048040030020042CrMo62058050040030018040CrM nMo55050045040025040CrNi*58051046042034020037CrNi3A*570500420300P 30040CrNiMoA62058054048042032035CrMoV640590500360300v 20038CrSi*63055052045040033038CrMoAiA680630530430320200水冷回火45B550450作彈簧回火50B420?40036028040Mn B*65045040MnVB60046045CrNi*

4、570500430360280230v 16065620550500450380300230v 200以下為彈簧鋼7062055050045038031023085620550500450380P 33025065Mn660600520440380300230v 17055SiM n55049060Si2 MnA620600550520470P 42038018050CrM n58050045040033060Si2CrV46042030W4Cr2VA550-650 C 回火GCr6550500460400300250v 200以下為軸承鋼GCr9550500460410350270v 180

5、GCr15680580530480420P 380270v 180GCr9Si Mn420350280v 200GCr15Si Mn480420350280v 180Cr6WV700650600540450250v 180以下為工具鋼T7(A)580530470420370320250< 160、模具鋼T8(A):580530470420370P 332250T10(A)580540490430380340250< 200T12(A)5805404904303803402509Mn2:4003402809M n2V500400320250< 180Cr260053048042

6、03202309Cr2Mo(W)700± 10,工頻淬后,700系調(diào)質(zhì)溫度9SiCr6706205805204503803001006SiCr630590530450380280< 200Cr580530480420350280< 200SiCr440370< 250CrMn590540490430340280< 180CrWM n640600540480420350280170Cr12650600520470P 250< 1000C淬火750700650600550> 1000 r淬火Cr12MoV740670620570530380< 180960-1030 C淬火700710650610550(二次硬化峰值1050-1130 C 淬火對應回火溫度)W350300240< 160W330P 280220CrW5620550500450400320270< 2009CrWM n620570520470370250< 1806SiM nV6005304704005CrMnMo580520470380r 250< 2005CrNiMo700

溫馨提示

  • 1. 本站所有資源如無特殊說明,都需要本地電腦安裝OFFICE2007和PDF閱讀器。圖紙軟件為CAD,CAXA,PROE,UG,SolidWorks等.壓縮文件請下載最新的WinRAR軟件解壓。
  • 2. 本站的文檔不包含任何第三方提供的附件圖紙等,如果需要附件,請聯(lián)系上傳者。文件的所有權(quán)益歸上傳用戶所有。
  • 3. 本站RAR壓縮包中若帶圖紙,網(wǎng)頁內(nèi)容里面會有圖紙預覽,若沒有圖紙預覽就沒有圖紙。
  • 4. 未經(jīng)權(quán)益所有人同意不得將文件中的內(nèi)容挪作商業(yè)或盈利用途。
  • 5. 人人文庫網(wǎng)僅提供信息存儲空間,僅對用戶上傳內(nèi)容的表現(xiàn)方式做保護處理,對用戶上傳分享的文檔內(nèi)容本身不做任何修改或編輯,并不能對任何下載內(nèi)容負責。
  • 6. 下載文件中如有侵權(quán)或不適當內(nèi)容,請與我們聯(lián)系,我們立即糾正。
  • 7. 本站不保證下載資源的準確性、安全性和完整性, 同時也不承擔用戶因使用這些下載資源對自己和他人造成任何形式的傷害或損失。

評論

0/150

提交評論